Defects Caused by Improper Cooling after Forging

2024-07-05
Defects caused by improper cooling after forging


Cooling cracks:


The cracks are smooth and slender, sometimes in the form of mesh cracks. High magnification observation: martensitic structure appears near the crack, and there is no trace of plastic deformation. It mostly occurs on martensitic steel forgings. Due to the rapid cooling after forging, large thermal stress and structural stress are generated. Slow cooling in a sandpit or slag around 200°C can prevent such cracks.

Cooling deformation:

Large, thin-walled, thin-ribbed frame members, warping deformation during post-forging cooling. It is caused by the interaction of residual stress generated in forging and stress caused by uneven cooling. Annealing immediately after forging can prevent such defects.

475℃ brittle crack:

Surface cracks appear when ferritic stainless steel is cooled too slowly after forging, and the residence time is too long in the temperature range of 400-520 °C. Due to the long residence time at 400-520 °C, a special substance is precipitated and brittleness is caused. Fast cooling at 400-520°C can prevent cracks.

Mesh Carbide:

Carbides are precipitated in the form of a network along the grain boundaries, which reduces the plasticity and toughness of the forgings. This defect is often seen in steel forgings with high carbon content. Due to the slow cooling after setting, the carbides can be folded along the grain boundaries, which makes the forgings easy to crack during quenching and deteriorates the performance of the parts.



ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.


主站蜘蛛池模板: 烟台市| 文成县| 旺苍县| 大同市| 广东省| 寿阳县| 布尔津县| 宁陕县| 溧阳市| 时尚| 额济纳旗| 进贤县| 凤台县| 达州市| 营山县| 华安县| 枞阳县| 洛川县| 麟游县| 宁津县| 新营市| 沛县| 山东省| 深水埗区| 泌阳县| 福海县| 资阳市| 水城县| 西林县| 贵州省| 阿拉尔市| 澄城县| 姜堰市| 茶陵县| 太原市| 丹棱县| 渑池县| 竹溪县| 韶山市| 榆中县| 渭源县|